Data of single Layer

E11  [MPa]

136000

E22  [MPa]

9400

E33  [MPa]

9400

v12

0.3

v13

0.3

v21

0.020735

v3

0.5

v31

0.020735

v32

0.5

G12 [MPa]

5400

G13 [MPa]

5400

G21 [MPa]

 

G23 [MPa]

3133

G31[MPa] (= )

5400

G32 [MPa]

 

ρ [kg/m3]

1500

 

Smeared Properties of the Laminate, quasi-isotropic, [0/90/-45/45]sym

 [MPa]

52889

 [MPa]

52889

 [MPa]

9400

E11

0.30402

E22

0.3

E33

0.30402

v12

0.5

v13

0.05332

v21

0.08885

G12  [MPa]

20279

G13  [MPa]

20279

G21[MPa]

 

.. [MPa]

17630

[MPa] (= )

20279

 [MPa]

 

ρ [kg/m3]

1500

Thermal expansion

 

Specific heat

 

Damping

 

Failure criteria

max. strain 0.2 %

« May 2012 »
Su Mo Tu We Th Fr Sa
1 2 3 4 5
6 7 8 9 10 11 12
13 14 15 16 17 18 19
20 21 22 23 24 25 26
27 28 29 30 31
 

Powered by Plone CMS, the Open Source Content Management System

This site conforms to the following standards: